Chemical composition in % for grade BrB2 ( БрБ2 )
Fe |
Si |
Ni |
Al |
Cu |
Pb |
Be |
Impurity |
max 0.15 |
max 0.15 |
0.2 - 0.5 |
max 0.15 |
96.9 - 98 |
max 0.005 |
1.8 - 2.1 |
all 0.5 |
Comment:
Cu is a basis; the percentage of
Cu is given approximately.
Mechanical properties under Т=20oС for grade BrB2 ( БрБ2 )
Assortment |
Dimension |
Direct. |
sв |
sT |
d5 |
y |
KCU |
Heat treatment |
- |
mm |
- |
MPa |
MPa |
% |
% |
kJ / m2 |
- |
Wire, GOST 15834 - 77 |
|
|
343-686 |
|
15-60 |
|
|
|
Wire, GOST 15834 - 77 |
|
|
735-1372 |
|
|
|
|
|
Strip, GOST 1789-70 |
|
|
390-590 |
|
20-30 |
|
|
|
Strip, GOST 1789-70 |
|
|
590-930 |
|
2.5 |
|
|
|
soft , GOST 1789-70 |
|
|
400-600 |
196-344 |
40-50 |
|
|
|
hard , GOST 1789-70 |
|
|
600-950 |
588-930 |
2-4 |
|
|
|
Brinell hardness for BrB2 ( БрБ2 ) , Bar GOST 15835-70 |
HB 10 -1 = 100 - 150 MPa |
Brinell hardness for BrB2 ( БрБ2 ) , Bar GOST 15835-70 |
HB 10 -1 = 150 MPa |
Technological properties of the material BrB2 ( БрБ2 ) .
Melting temperature : |
955 °C |
Forging temperature : |
750 - 800 °C |
Annealing temperature : |
530 - 650 °C |
Physical properties for grade BrB2 ( БрБ2 )
T |
E 10- 5 |
a 10 6 |
l |
r |
C |
R 10 9 |
Grade |
MPa |
1/Grade |
Watt/(m·Grade) |
kg/m3 |
J/(kg·Grade) |
Ohm·m |
20 |
1.31 |
|
84 |
8200 |
|
70 |
100 |
|
16.6 |
|
|
419 |
|
Equivalent steels for grade BrB2 ( БрБ2 )
Warning! Indicated both exact and nearest equivalents.
USA |
Germany |
Japan |
- |
DIN,WNr |
JIS |
|
|
|